Glaze test for Turnidge/MFE Crystalline Glaze, cone 6, ox.



Source: Clayart, Bill Sheppard

Credited to:



Fired on mid fire white stoneware.



Firing ramp with an electric controller is:
100c p/h to 600c (212f - 1112f)
150c p/h to 1140c (302f - 2084f)
80c p/h to 1220c (176f - 2228f)
15 min. soak
cool down max. to 900c (1652f)
Hold 1 hour
Shut off kiln



Recipe:

50 Frit 3110 subbed local high boron frit which is half the glaze,
but that is what I have.

22.5 Zinc Oxide

22.5 Silica

5 Lithium Carb.



Note: All raw materials are measured up or down to the nearest half
decimal. Colorants or additives to a 100 gram batch are measured in percent
to the 100 gram batch.



Results:

Gloss, transparent glaze with stark white streaking. White cyrstals
developed around edges of test tile, which is an extruded square tube.
Runny. Glaze is crazed.



With Added Nikkel, 2 percent:

Gloss, transparent glaze with softer white and pink streaking. Bright blue
crystals along edges of test tile and bottom dipping line. Runny. Glaze is
not crazed.



Regards from Alisa in Denmark