Here are three recipes for c.5. 6.

All based on US recipes I know work. These recipes used Ferro
Frits. I adapted them to use your two frits. I "found" that in two
cases my recipe adaptation resulted in just about (mais ou menos) an equa=
l
amount of each frit.

I would test them and then add some opacifiers--maybe a little rutile as
well as opacifier....The first two are based on glazes that had titanium,
rutile, tin, or zirconium added. All were figured on my GlazeMaster=99
program.

I would be very grateful if you tested these and let me know how they tur=
n
out. Many thanks. NOTHING is as exciting as the international characte=
r
of pottery...


Recipe Name: heloisa #1


Amount Ingredient
29 braz.093
26.2 brazilian 096
11.1 Whiting
7.5 Zinc Oxide
15.7 Kaolin--
10.5 Flint

Unity Oxide
.197 Na2O
.003 K2O
.005 MgO
.532 CaO
.264 ZnO
.287 Al2O3
.344 B2O3
.002 Fe2O3
2.443 SiO2


heloisa #2


Amount Ingredient
25.6 braz.093
24.4 brazilian 096
18.2 Whiting
22.7 Kaolin--9.1
9.1 Flint

Unity Oxide
.199 Na2O
.004 K2O
.008 MgO
.79 CaO

.386 Al2O3
.348 B2O3
.003 Fe2O3

2.638 SiO2


heloisa's clear



Amount Ingredient
14.2 braz.093
57 brazilian 096
5.3 Whiting
14 Kaolin--EPK
9.5 Flint


Unity Oxide
.379 Na2O
.004 K2O
.008 MgO
.609 CaO
1.000 Total

.359 Al2O3
.658 B2O3
.002 Fe2O3

3.57 SiO2



Lili Krakowski
Be of good courage


Lili Krakowski
Be of good courage

Heloisa Nunes on fri 9 jun 06


Dear Lili,

Thank you so much for the recipes. I look forward to trying them the next
weeks and I will get back to you with the results.
I am trying to reach Ferro and ask about a high boron frit. n/'/tf
I also had no luck reaching you (my emails also returned). I will try and
find out what is happening with my server and how I can reach you directly
next time.
I don't feel I can thank you enough!

All the best,
Heloisa Nunes
helonunes@hnet.com.br