annapoorna sitaram on wed 14 jun 06
hello
i have a clay body that fires a horrible pale pastel.
I am trying to do some slip work on raw ware so i need a white slip.
Is it possible to make up a white slip by adding tin or what else?
I have tried talc ware it is not for me i need a more plastic body.
thanking all of you in advance,
annapoorna sitaram
from bangalore
india
Cindy Gatto on thu 15 jun 06
I use a recipe called old reliable slip it is supposedly from Alfred It is
rated for ^06 -^03 but I use it at ^6 as well. It works great I have never seen
any problem at all with it and it used with a variety of clays and works
from leather hard to bone dry
om-4 ball 40
EPK 20
neph sye 10
talc 15
flint 15
Cindy Gatto & Mark Petrin
The Mudpit
228 Manhattan Ave
Brooklyn, NY 11206
718-218-9424
_www.mudpitnyc.com_ (http://www.mudpitnyc.com/)
mudpitnyc@aol.com
| |
|