Mike Gordon on wed 18 oct 06
Dustin wrote..
i was wondering if anyone has the recipe for matt long's claybody? i
have
a Joe Christensen cup made from matt long's porcelain and it seems to
flash very well. any info on the recipe would be greatly appreciated.
Dustin,
here is the recipe from his handout I received last summer,
Porcelain cone 10 and up
Grolleg...........................55
Silica.............................27
Custer............................15
Calcined Alumina............3
Vee gum T......................2
His web site is .... www.fullvictory.com
Email.....mattlong@ufl.edu
Mike Gordon
Dustin Harris on thu 19 oct 06
thank you mike i appreciate the info
dustin
| |
|