dominique michaels on sun 4 feb 07


MINNESOTA MONET

I lost my glaze recipe for soto amber. Does any one
know this recipe. It's for cone 6 firing. I can't do
my next firing until I make another batch. I would
be so greatful to anyone that could email this to me.

thank you,
Minnesota



____________________________________________________________________________________
Yahoo! Music Unlimited
Access over 1 million songs.
http://music.yahoo.com/unlimited

Sandi Taylor on sun 4 feb 07


Hi Minnesota,
This is the recipe that I have in my notebook.
At one time I did a lot of testing in ^6. I hope this is helpful.
Soto Amber ^6
Ferro Frit 3124 32.2
Kona F4 25.8
Silica 19.4
Whiting 12.9
Tile#6 4.85
EPK 4.85
R.I.O. 3.0
Copper Carb .75

Sandi Taylor
----- Original Message -----
From: "dominique michaels"
To:
Sent: Sunday, February 04, 2007 10:31 AM
Subject: cone 6 recipe anyone?


> MINNESOTA MONET
>
> I lost my glaze recipe for soto amber. Does any one
> know this recipe. It's for cone 6 firing. I can't do
> my next firing until I make another batch. I would
> be so greatful to anyone that could email this to me.
>
> thank you,
> Minnesota
>
>
>
> ____________________________________________________________________________________
> Yahoo! Music Unlimited
> Access over 1 million songs.
> http://music.yahoo.com/unlimited
>
> ______________________________________________________________________________
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
> melpots@pclink.com.

sacredclay on sun 4 feb 07


Sweet ladies, you can't just post that and not give some of us a clue
as to what it looks like? Post a pix so I can see and is it R or Ox.?
I'm assuming Ox. I religiously write down all of the recipes that I
see on the list except for low fire. thanks, Kathryn in NC --- In
clayart@yahoogroups.com, Sandi Taylor wrote:
>
> Hi Minnesota,
> This is the recipe that I have in my notebook.
> At one time I did a lot of testing in ^6. I hope this is helpful.
> Soto Amber ^6
> Ferro Frit 3124 32.2
> Kona F4 25.8
> Silica 19.4
> Whiting 12.9
> Tile#6 4.85
> EPK 4.85
> R.I.O. 3.0
> Copper Carb .75
>