search  current discussion  categories  wanted/for sale - wanted 

looking for ^9 glazes

updated mon 30 sep 96

 

Anne Lythgoe, OP on wed 25 sep 96

Our community art center glazing class is on the lookout for some nice cone 9
reduction glazes, especially celedon...any suggestions or receipes out there?

Anne Lythgoe, OP

103533.1260@compuserv.com

marilyn fenton on thu 26 sep 96

try:
custer spar 350
talc 50
whiting 200
OM#4 200
flint 200

RIO 1.5%

good firing range...you might have to adjust silica..or
not...we like crackled celedon