Sam Ewing on sun 4 jan 98
Hello All,
I'm just begining to get into making my own glazes. I'm looking for a good
matt-finish base glaze for cone 6 oxidation firing.
Any recipes and suggestions would be greatly appreciated.
Thanks,
Rosalie
Bryan Stecker on tue 6 jan 98
Try this.
Matt base ^6
Dolomite 19
Whiting 3
Neph Sy 35
Ball Clay 19
Silica 19
Nice results with a variety of colorants.
Anne Stecker
rekcets@open.org
Sam Ewing wrote:
> ----------------------------Original message----------------------------
> Hello All,
>
> I'm just begining to get into making my own glazes. I'm looking for a good
> matt-finish base glaze for cone 6 oxidation firing.
>
> Any recipes and suggestions would be greatly appreciated.
>
> Thanks,
>
> Rosalie
| |
|