search  current discussion  categories  wanted/for sale - wanted 

looking for cone 6 oxidation/copper?

updated wed 4 oct 00

 

cHuCk on tue 3 oct 00


How do you feel about the Cu in it....is that Copper Carb or Oxide?

Do you use this for functional liner glaze...just curious.

Cwag

> Andie,
> Here is a recipe I really like. It came from Ceramics Monthly,November
> 91, page 53. The contributors name escapes me, but his initials are M.F.
>
> M.F. Bold Black cone 4 to 6
>
> Dolomite 10.0
> Lith carb 2.0
> Zinc oxide 1.0
> Frit #l4 Hommel 20.5 (I used Ferro 3l34)
> Barnard Clay40.0
> EPK 13.5
> Flint l3.0
>
> add CO carb 3.0
> Cu carb 2.0
> Rutile 1.0
> Titanium dioxide 3.0
>
>
> Hope this helps, Mia in warm ABQ
>
>
____________________________________________________________________________
__
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.