search  current discussion  categories  wanted/for sale - wanted 

looking for coleman black cone 10

updated fri 3 dec 04

 

Mishy Lowe on wed 1 dec 04


Hey all, Long time since I visited clayart, been in
the throes of divorce and trying to remain financially
functional amidst it all...yikes!

Had a computer crash and my glaze files are locked and
inaccessible for now...and I am in need of a recipe
for cone ten black, Susan Filley shared it when she
did a workshop here a few years ago, I think it's Tom
Coleman's black, also published in Clay Times in
Jan/Feb 2003 (where *is* my copy of that issue?)

Anyone willing to share, or look it up for me?

Thanks in advance...and I've missed you all :-)
Life is good,
Mishy (soon to be Mishy Katz)

=====
Mishy

www.desertdragonpottery.com
Desert Dragon Pottery 602 690 6956

__________________________________________________
Do You Yahoo!?
Tired of spam? Yahoo! Mail has the best spam protection around
http://mail.yahoo.com

Krista Peterson on thu 2 dec 04


>Had a computer crash and my glaze files are locked and
>inaccessible for now...and I am in need of a recipe
>for cone ten black, Susan Filley shared it when she
>did a workshop here a few years ago, I think it's Tom
>Coleman's black, also published in Clay Times in
>Jan/Feb 2003 (where *is* my copy of that issue?)


Hey Mishy!

I have a bunch of Tom Coleman Black and Tenmoku glazes. Do you know which one? I have:

F. Black
S.J. Black
Ash Black
Brown Matt Black
Black Jack
Teadust Black
Chun-like Black and many more

I have the booklet he sold at a workshop at PCC so any glaze I can pass along.

Let me know~!
Take care
Krista

Rosanne on thu 2 dec 04


TOM COLEMAN'S BLACK

Custer Feldspar 32.90
Silica 32.69
Whiting 15.38
OM-4 Ball Clay 9.62
EPK 9.62

add:
Red Iron Oxide 8.0
Cobalt Carbonate 3.8

John Britt on thu 2 dec 04


Mishy,

I think it is also known as Filley Black:

G-200 32.5
Whiting 15.5
Silica 32.5
Ball Clay 19.5

Cobalt Carbonate 5.0
Red Iron Oxide 10.0

Hope that helps,

John Britt
www.johnbrittpottery.com

John Britt on thu 2 dec 04


Mishy,

I think it is also known as Filley Black

G-200